Hot Deformation Behavior of Ni80A Superalloy During Non-Isothermal Side Pressing

نویسندگان

  • M. Seyed Salehi Department of Materials Science and Engineering, K. N. Toosi University of Technology, Tehran, Iran
  • N. Anjabin Department of Materials Science and Engineering, School of Engineering, Shiraz University, Shiraz, Iran
  • R. Mansoori Research and Development Center, Turbine Machine Middle East Co., Tehran, Iran
چکیده مقاله:

In the present study, the microstructural changes of a Nickel based superalloy Nimonic80A during a non-isothermal deformation were studied. Therefore, microstructure evolutionduring hot side pressing test was predicted with combined methods of finite element analysis andprocessing map of the material. The predicted results were validated through experimentalmicrostructural studies. The results show that the distribution of deformation parameters (i.e.strain, strain rate, and temperature) is non-uniform in the deformed samples. The severity of thisnon-uniformity depends on the amount of sample reduction. High reduction value at one stepforging can cause flow localization and non-uniform dynamic recrystallization, which results theformation of adiabatic shear bands, while using the lower reduction value at each forging step,leads to more uniformly distribution of the deformation parameters and thus uniform the dynamicrecrystallization with the stable flow. Hence the workability and microstructure of the Nimonic80A alloy are mainly depends on the deformation path.

Download for Free

Sign up for free to access the full text

اگر عضو سایت هستید لطفا وارد حساب کاربری خود شوید

منابع مشابه

hot deformation behavior of ni80a superalloy during non-isothermal side pressing

in the present study, the microstructural changes of a nickel based superalloy nimonic80a during a non-isothermal deformation were studied. therefore, microstructure evolutionduring hot side pressing test was predicted with combined methods of finite element analysis andprocessing map of the material. the predicted results were validated through experimentalmicrostructural studies. the results ...

متن کامل

Hot Deformation Behavior and Pulse Current Auxiliary Isothermal Forging of Hot Pressing Sintering TiAl Based Alloys

This paper focuses on the fabrication of as-forged Ti46.5Al2Cr1.8Nb-(W, B) alloy via pulse current auxiliary isothermal forging (PCIF). The starting material composed of near gamma (NG) microstructure was fabricated by adopting pre-alloyed powders via hot pressing sintering (HPS) at 1300 °C. Isothermal compression tests were conducted at a strain rate range of 0.001-0.1 s-1 and a temperature ra...

متن کامل

Prediction of the Hot Compressive Deformation Behavior for Superalloy Nimonic 80A by BP-ANN Model

Abstract: In order to predict hot deformation behavior of superalloy nimonic 80A, a back-propagational artificial neural network (BP-ANN) and strain-dependent Arrhenius-type model were established based on the experimental data from isothermal compression tests on a Gleeble-3500 thermo-mechanical simulator at temperatures ranging of 1050–1250 ̋C, strain rates ranging of 0.01–10.0 s ́1. A comparis...

متن کامل

Effects of Carbon on the Microstructure and Hot Deformation Behavior

The effects of carbon content on the dynamic and static softening mechanisms of Ti microalloy steels were investigated both in ferrite and austenite regions. &#10The results obtained showed that recrystallization rate decreased as the percentage of carbon content was increased from 0.0035 to 0.110. This is due to the Ti(CN) and TiC precipitates and also the free carbon content. In the ferrite r...

متن کامل

Effects of Carbon on the Microstructure and Hot Deformation Behavior

The effects of carbon content on the dynamic and static softening mechanisms of Ti microalloy steels were investigated both in ferrite and austenite regions. The results obtained showed that recrystallization rate decreased as the percentage of carbon content was increased from 0.0035 to 0.110. This is due to the Ti(CN) and TiC precipitates and also the free carbon content. In the ferrite reg...

متن کامل

Microstructural Evaluation of Ti-6AL-4V Alloy during Hot Deformation

Among the titanium alloys, Ti-6Al-4V is the most widely used. In the present work, the uniaxial hot compressive behavior of Ti-6Al-4V has been investigated under constant strain rates. A series of dilatometery experiments were carried out to determine the transformation temperatures at different cooling rates. Specimens were homogenized at 1050 °C for 10 minutes followed by fast cooling to dif...

متن کامل

منابع من

با ذخیره ی این منبع در منابع من، دسترسی به آن را برای استفاده های بعدی آسان تر کنید

ذخیره در منابع من قبلا به منابع من ذحیره شده

{@ msg_add @}


عنوان ژورنال

دوره 2  شماره 1

صفحات  18- 29

تاریخ انتشار 2015-04-01

با دنبال کردن یک ژورنال هنگامی که شماره جدید این ژورنال منتشر می شود به شما از طریق ایمیل اطلاع داده می شود.

میزبانی شده توسط پلتفرم ابری doprax.com

copyright © 2015-2023